How Do SA515 Grade 70 and SA516 Grade 70 Differ in Service?

SA515 Grade 70 vs SA516 Grade 70
Picture of Chiranjiv Steel Centre

Chiranjiv Steel Centre

Share this read
Table of contents
Pressure vessel plates
Need A516 Grade 70 plates with full certification?
1 min
Use AI to summarize this article

SA515 Grade 70 and SA516 Grade 70 are both carbon steel plates for welded pressure vessels, and their strength requirements are identical. Same tensile range, same minimum yield, same elongation. On a datasheet they are indistinguishable.

The difference is grain structure, and it decides where each plate belongs. SA515 is made to a coarse grain practice for intermediate and higher temperature service. SA516 is made to a fine grain practice for moderate and lower temperature service. Coarse grain resists creep and graphitization during long exposure to heat. Fine grain resists brittle fracture in the cold. You cannot have both in the same plate.

This blog explains how the two behave in service rather than on paper. It covers grain structure and chemistry, what happens at high and low temperature, why both carry the same allowable stress in the ASME code, whether the plate you receive is actually coarse grained, and why SA516 has largely replaced SA515 in modern practice.

SA515 Grade 70 vs SA516 Grade 70: Comparison Table

  SA515 Grade 70 SA516 Grade 70
Specification title Pressure vessel plates, carbon-silicon steel, for intermediate and higher temperature service Pressure vessel plates, carbon steel, for moderate and lower temperature service
Grain practice Coarse grain Fine grain, required
Tensile strength 485–620 MPa (70–90 ksi) 485–620 MPa (70–90 ksi)
Yield strength, minimum 260 MPa (38 ksi) 260 MPa (38 ksi)
Elongation in 200 mm, minimum 17% 17%
Carbon, maximum 0.31% and above, by thickness 0.27 to 0.31%, by thickness
Manganese 0.90% maximum, no minimum 0.85–1.20%
Notch toughness Lower Higher
Creep resistance Better Lower
Suited to Elevated temperature Ambient and below
Availability today Limited Widely stocked

Same Strength, Different Steel

Both grades specify 485 to 620 MPa tensile strength, a minimum yield of 260 MPa, and minimum elongation of 17% over 200 mm or 21% over 50 mm. Nothing in the mechanical test results will tell you which plate you are holding.

That is the trap in this comparison. Buyers see matching numbers and conclude the plates are interchangeable, but the tensile test measures strength at room temperature over a few minutes. Neither the creep behaviour of a vessel running at 450 °C for twenty years nor the brittle fracture risk of a vessel starting up on a winter morning shows up in it.

The full set of certified figures, and what to check them against, is covered in the mechanical properties of A516 Grade 70 plate.

Grain Structure: The Real Difference

Coarse grain vs fine grain steel

Grain size describes how large the individual crystals are within the steel, and it is controlled during steelmaking through deoxidation practice and the residual elements left in the melt.

Coarse grain means larger crystals with less total grain boundary area. Grain boundaries are where creep deformation concentrates at high temperature, so fewer of them slows creep down. Coarse grain also resists graphitization better during long heat exposure.

Fine grain means smaller crystals with more grain boundary area. Those boundaries interrupt a running crack, so a crack has to change direction repeatedly instead of travelling straight through. That is what raises fracture toughness and lowers the temperature at which the steel turns brittle.

The two benefits pull in opposite directions, which is why two specifications exist rather than one. SA516 requires fine grain practice. SA515 was written around coarse grain for the opposite reason.

Chemical Composition Comparison

Element SA515 Grade 70 SA516 Grade 70
Carbon 0.31% max at thin sections, rising with thickness 0.27% max at thin sections, rising to 0.31%
Manganese 0.90% maximum only 0.85–1.20%
Silicon 0.15–0.40% 0.15–0.40%
Phosphorus 0.035% max 0.025% max
Sulphur 0.035% max 0.025% max

Three points explain the behaviour difference.

SA515 carries more carbon. It reaches the same 485 MPa tensile minimum largely through carbon, which suits high temperature strength but reduces toughness.

SA515 sets no manganese minimum. It caps manganese at 0.90% and requires none. SA516 requires at least 0.85% on every plate, because manganese contributes both strength and toughness. This is a substantial difference in how the two specifications reach the same strength.

SA516 is the cleaner steel. Phosphorus and sulphur are capped at 0.025% against 0.035% in SA515. Sulphur forms elongated inclusions that reduce through-thickness ductility, which matters more in the cold.

Note the specification titles too. SA515 is a carbon-silicon steel, with silicon deliberately part of its identity for elevated temperature strength. SA516 is simply a carbon steel.

Service Temperature: Where Each Belongs

SA515 Grade 70 is written for intermediate and higher temperature service. In practice that means vessels and boiler components operating well above ambient, where the coarse grain structure earns its place and where the material stays comfortably above its ductile to brittle transition temperature throughout operation.

SA516 Grade 70 is written for moderate and lower temperature service. It handles ambient duty and, in the normalized condition with impact testing specified, service down to −46 °C and beyond.

The dividing question is simple. Does your vessel spend its life hot, or does it see ambient and colder conditions including start-up, shutdown and upset? Most process vessels see the second, which is why SA516 dominates.

Creep Resistance at High Temperature

High temperature pressure vessel

Creep is slow permanent deformation under sustained load at elevated temperature. It is not a strength problem in the usual sense, since the stress may be well below yield. It is a time problem, and it accumulates over years.

Creep concentrates at grain boundaries, so a coarse grained steel with fewer boundaries creeps more slowly than a fine grained one under the same conditions. That is the technical case for SA515 in hot service.

For a vessel running for decades at elevated temperature, that difference compounds. For a vessel running at ambient, it is irrelevant, because creep is not a mechanism at those temperatures.

Graphitization and Long Term Heat Exposure

Graphitization is the second reason SA515 exists, and it is less well known than creep.

In carbon steels held for long periods above roughly 425 °C, the iron carbide in the microstructure can slowly decompose into nodules of free graphite. Graphite has almost no strength, so these nodules act as internal defects and the steel loses toughness. The damage is cumulative and cannot be reversed in service.

Susceptibility depends partly on how the steel was deoxidised and on its grain structure. Coarse grained silicon-killed steel resists graphitization better than fine grained aluminium-killed steel, which is why SA515 was preferred for long-term high temperature duty in older plant.

Two practical notes. Graphitization needs both temperature and time, so it concerns vessels in continuous hot service rather than ones seeing occasional excursions. And it is one reason carbon steel of any kind is a poor choice for sustained service much above 425 °C, where alloy steels such as A387 are usually the right answer instead.

Notch Toughness and Brittle Fracture

Charpy impact test steel plate

Every carbon steel has a temperature below which it stops failing in a ductile way and starts failing suddenly and without warning. That point is the ductile to brittle transition temperature, and grain structure moves it.

Fine grain lowers the transition temperature, so a fine grained plate stays tough further into the cold. Coarse grain raises it, so a coarse grained plate becomes brittle at a higher temperature than an equivalent fine grained one.

This is the whole reason SA515 is unsuitable for ambient and low temperature vessels. Above its transition temperature it behaves perfectly well, which is why it is acceptable for hot service. Below it, an impact or a pressure surge can cause a fast fracture with no prior yielding.

Charpy V-notch impact testing is a supplementary requirement in both specifications, so neither is tested unless you ask. The difference is what happens when you do. SA516 Grade 70, particularly normalized, meets demanding requirements reliably. SA515 has no fine grain guarantee behind it, and mills will often decline to certify it at low temperature.

Why Both Carry the Same Allowable Stress

Here is a point that puzzles engineers meeting these grades for the first time.

ASME Section VIII Division 1 sets allowable stress as the lower of minimum tensile strength divided by 3.5, or two thirds of minimum yield strength. Both grades have the same 70 ksi minimum tensile and the same 38 ksi minimum yield, so both come out at the same allowable stress of 20.0 ksi at ambient temperature. The published maximum use temperature in Section II Part D is also the same for both.

So the code does not distinguish between them on either allowable stress or temperature limit. If you were choosing purely from the stress tables, they would look identical.

What the tables cannot express is long-term degradation. Creep and graphitization develop over years, and brittle fracture depends on a transition temperature that no allowable stress value captures. The material choice sits with the design engineer’s judgement about service conditions over the life of the vessel, not with the stress table alone.

Always read current values from the Section II Part D tables for your code edition rather than relying on figures quoted online.

Is SA515 Actually Coarse Grained?

Steel plate mill test certificate

This deserves attention, because it undermines the assumption most comparisons are built on.

SA515 is intended for coarse grain material, but the specification does not prohibit fine grain practice. Modern steelmaking is far more uniform than it was when the specification was written, and experienced engineers have long observed that plate supplied as SA515 is often made to fine grain practice, detectable from the aluminium, vanadium and niobium residuals on the analysis.

The practical consequence is significant. If you specify SA515 expecting coarse grain creep resistance and graphitization resistance, and the mill supplies fine grained material, you have not got what the design assumed. The plate will pass every test on the certificate.

Two steps protect you. Discuss the grain practice explicitly with the mill at enquiry stage rather than assuming it follows from the specification, and check whether a supplementary requirement in the current edition can be invoked to guarantee it. Then confirm on the certificate what was actually supplied, using the residual element analysis as a cross-check. What to look for field by field is covered in our guide to the A516 Grade 70 mill test certificate, and the same reading applies to SA515.

Weldability and Fabrication

Welding pressure vessel plate

Both grades weld with low-hydrogen consumables and standard carbon steel procedures.

SA516 Grade 70 is the more forgiving of the two. Its manganese content contributes toughness in the heat-affected zone, and its lower carbon at comparable thicknesses gives a slightly lower carbon equivalent.

SA515 Grade 70 needs a little more care as thickness rises, because of its higher carbon and the absence of a manganese minimum. Preheat and interpass temperature control matter, and the heat-affected zone in a coarse grained steel is inherently less tough than in a fine grained one.

Post-weld heat treatment requirements follow the ASME rules for P-No. 1 material in both cases, based on thickness and service rather than on the choice between these two grades.

Why SA516 Has Largely Replaced SA515

SA515 is now uncommon. Several things drove that.

Most vessels are not hot vessels. The great majority of process, storage and separation equipment operates at ambient or below, where fine grain toughness is what matters.

Modern codes ask more about toughness. Impact testing requirements have tightened considerably, and SA516 answers them where SA515 cannot.

SA516 can substitute upward but not the reverse. Where the service is not genuinely high temperature, SA516 does everything SA515 does and more.

Availability compounds itself. SA516 Grade 70 is stocked worldwide in a wide thickness range. SA515 is often a mill order with longer lead time and a limited size range, which pushes more designers toward SA516, which in turn thins SA515 stock further.

Genuinely hot service usually needs alloy steel anyway. Above roughly 425 °C, chromium-molybdenum grades such as A387 are typically the right choice, which narrows the window where SA515 is the best answer to a fairly small band.

Can One Replace the Other?

SA516 Grade 70 in place of SA515 Grade 70 is usually acceptable and is routinely done. Mechanical requirements are identical, SA516 is the cleaner steel, and its fine grain gives better toughness. The exception is genuine long-term high temperature service, where the coarse grain creep and graphitization resistance was the reason SA515 was specified in the first place. Substituting there removes the property the designer wanted.

SA515 Grade 70 in place of SA516 Grade 70 should not be done. It fails on notch toughness, it is unsuitable for ambient and low temperature service, and it cannot support impact testing requirements.

In both directions the substitution is a design engineer’s decision, not a purchasing one, and it should be approved in writing before the plate is cut. Welding procedures should be reviewed at the same time.

Applications

SA516 Grade 70 pressure vessels

SA515 Grade 70 suits equipment in sustained elevated temperature service, including higher temperature pressure vessels, certain boiler components, steam service equipment, and older plant where the original design specified it and replacement material must match.

SA516 Grade 70 suits pressure vessels and reactors in refinery and petrochemical service, storage tanks to API 650 and API 620, heat exchanger shells and channels, LPG and ammonia storage, cold-service equipment, and sour service vessels with HIC testing. If your project calls for SA516 Grade 70 plate, it is usually because the service is ambient or below and toughness is the governing property.

Frequently Asked Questions

What is the main difference between SA515 Grade 70 and SA516 Grade 70?

Grain structure, not strength. Both have identical tensile, yield and elongation requirements. SA515 is made to a coarse grain practice for intermediate and higher temperature service, where it resists creep and graphitization. SA516 is made to a fine grain practice for moderate and lower temperature service, where it resists brittle fracture.

Which is better, SA515 Grade 70 or SA516 Grade 70?

Neither is better in general terms, since they suit different service conditions. For ambient and low temperature vessels, which covers most equipment, SA516 Grade 70 is the correct and safer choice. For sustained high temperature duty, SA515 was written for the job, though above roughly 425 °C an alloy steel is often more appropriate than either.

Can SA516 Grade 70 replace SA515 Grade 70?

Usually yes, and it is commonly done, since SA516 meets every mechanical requirement of SA515 and is a cleaner, tougher steel. The exception is genuine long-term high temperature service, where the coarse grain structure was the reason SA515 was chosen. Any substitution needs the design engineer’s written approval.

Why does coarse grain help at high temperature?

Creep deformation concentrates at grain boundaries, so a coarse grained steel with fewer boundaries creeps more slowly under sustained load at temperature. Coarse grained silicon-killed steel also resists graphitization better, which is the slow breakdown of iron carbide into weak graphite nodules during long heat exposure.

Do both grades have the same allowable stress?

Yes. Because both share the same minimum tensile and yield strength, ASME Section VIII Division 1 gives both the same allowable stress, and the published maximum use temperature is also the same. The code tables cannot express long-term creep, graphitization or brittle fracture behaviour, which is why material selection remains an engineering judgement rather than a table lookup.

Is SA515 always supplied with coarse grain?

Not necessarily. The specification is intended for coarse grain material but does not prohibit fine grain practice, and with modern steelmaking, SA515 plate is often produced fine grained. If the coarse grain structure is what your design depends on, discuss it with the mill at enquiry stage and confirm what was supplied on the certificate rather than assuming it follows from the specification.

Is SA515 Grade 70 suitable for low temperature service?

No. Its coarse grain structure raises the ductile to brittle transition temperature, so it can fail suddenly and without warning in the cold. For low temperature vessels, use normalized SA516 Grade 70 with Charpy impact testing specified at your minimum design metal temperature.

Why is SA515 rarely used now?

Most vessels operate at ambient or below, where toughness governs and SA516 is the better fit. Toughness requirements in modern codes have also tightened, SA516 can substitute for SA515 in most situations, and genuinely hot service usually calls for alloy steel. Together these have left SA515 with a narrow window and thin stock availability.

Which One to Specify

SA515 Grade 70 and SA516 Grade 70 are the same on paper and different in service. Identical strength figures, identical allowable stress, identical code temperature limit, and opposite metallurgy underneath.

The decision rests on one question. If the vessel spends its life hot and creep or graphitization over decades is the concern, SA515 was written for that duty, though above roughly 425 °C an alloy steel deserves consideration first. If the vessel sees ambient conditions or colder at any point, including start-up and shutdown, SA516 Grade 70 is the correct choice and its fine grain structure is exactly the property you need.

For most projects the answer is SA516 Grade 70. Where SA515 is genuinely required, confirm the grain practice with the mill rather than assuming the specification delivers it.

Found this useful? Share it.

Popular articles