Structural Steel vs Pressure Vessel Steel: A36 and A516 Grade 70 Compared

A36 vs A516 Grade 70
Picture of Chiranjiv Steel Centre

Chiranjiv Steel Centre

Share this read
Table of contents
Pressure vessel plates
Need A516 Grade 70 plates with full certification?
1 min
Use AI to summarize this article

they look similar enough that buyers reasonably ask whether one can stand in for the other. A36 is a structural steel written for buildings, bridges, frames and machinery. A516 Grade 70 is pressure vessel quality plate, written for welded vessels that contain pressure at moderate and lower temperatures.

The gap between them is not mainly about strength. It is about control. A516 tightens the chemistry, mandates fully killed steel and a fine grain practice, requires full heat traceability, and opens the door to impact testing and ultrasonic examination. A36 sets outer limits on composition and leaves the rest to the mill, because a beam carrying a floor load does not face the failure modes a pressure vessel does.

Below we compare the two on strength, ductility, chemistry, steelmaking practice, toughness and cost, then deal with the two substitution questions directly, including what the ASME code actually permits rather than what most articles claim it says.

A36 vs A516 Grade 70: Comparison Table

  ASTM A36 ASTM A516 Grade 70
Steel type Carbon structural steel Pressure vessel quality carbon steel
Written for Buildings, bridges, frames, machinery Welded pressure vessels and boilers
Tensile strength 400–550 MPa (58–80 ksi) 485–620 MPa (70–90 ksi)
Yield strength, minimum 250 MPa (36 ksi) 260 MPa (38 ksi)
Elongation in 200 mm, minimum 20% 17%
Elongation in 50 mm, minimum 23% 21%
Phosphorus, maximum 0.04% 0.025%
Sulphur, maximum 0.05% 0.025%
Steelmaking practice Killed required only above 40 mm Fully killed, fine grain, all thicknesses
Impact testing Not part of the specification Available as a supplementary requirement
ASME code status SA-36, permitted with restrictions SA-516, standard pressure vessel material
Relative cost Lowest Around 10 to 20% higher

What Pressure Vessel Quality Actually Means

Heat number markings on pressure vessel quality steel plate

The term PVQ appears constantly in plate trading and is rarely explained. It refers to plate produced and certified under a specification written for pressure containment, which brings four things a structural specification does not.

Controlled steelmaking. A516 requires fully killed steel and a fine austenitic grain practice on every plate. Killing removes dissolved oxygen so the plate solidifies without gas porosity. Fine grain is the main defence against brittle fracture.

Tighter impurity limits. Phosphorus and sulphur are capped at 0.025% each, against 0.04% and 0.05% in A36. Sulphur in particular forms elongated inclusions that harm through-thickness ductility and give hydrogen cracks a path to follow.

Full heat traceability. Every plate ties back to a specific heat of steel with its own certified test results, and the plate is marked accordingly.

A general requirements standard behind it. A516 sits on ASTM A20, which governs test methods, retesting, defect repair and the numbered supplementary requirements such as Charpy impact testing and ultrasonic examination. A36 has no equivalent framework of optional controls.

None of this makes A516 a better steel in the abstract. It makes it a controlled steel, which is what a code inspector needs before signing off on a vessel.

Strength Comparison

Measure A36 A516 Grade 70 Difference
Minimum yield 250 MPa 260 MPa 4% higher
Minimum tensile 400 MPa 485 MPa 21% higher

The yield strengths are close enough to be almost the same, which surprises people expecting a large gap. Where the two separate is tensile strength, and that matters more than it appears, because ASME Section VIII Division 1 derives allowable stress from minimum tensile strength divided by a design margin of 3.5. A516 Grade 70 carries a maximum allowable stress of 20.0 ksi at ambient temperature. A36 starts from a 58 ksi minimum tensile rather than 70 ksi, so its allowable stress works out roughly 17% lower. Published values should always be read from the Section II Part D tables for your code edition rather than calculated by hand.

One detail on A36 worth knowing: the 250 MPa minimum yield applies to plate up to 200 mm thick, and drops to 220 MPa above that. A516 Grade 70 holds 260 MPa at every thickness.

For the full set of certified figures behind Grade 70, including how the tensile ceiling works and what to check on a mill certificate, see the mechanical properties of A516 Grade 70 plate.

Ductility and Elongation

Tensile test specimens comparing steel plate ductility
Gauge length A36 A516 Grade 70
200 mm (8 in.) 20% minimum 17% minimum
50 mm (2 in.) 23% minimum 21% minimum

A36 is the more ductile of the two on both gauge lengths. Its lower carbon and lower manganese leave it softer and more forgiving in forming, which is one reason it remains popular for general fabrication and cold-formed parts.

This is the standard trade-off. The manganese that lifts A516 Grade 70 to 485 MPa tensile is the same addition that pulls its elongation down.

Chemical Composition Comparison

Element ASTM A36 >ASTM A516 Grade 70
Carbon 0.25 to 0.29% max, by thickness 0.27 to 0.31% max, by thickness
Manganese Not required below 20 mm, then 0.80–1.20% 0.85–1.20% at all thicknesses
Phosphorus 0.04% max 0.025% max
Sulphur 0.05% max 0.025% max
Silicon 0.40% max 0.15–0.40%

Read the manganese row carefully, because it shows the difference in philosophy. A36 sets no manganese requirement at all on plate up to 20 mm, so a thin A36 plate may contain very little. A516 Grade 70 sets a minimum of 0.85% on every plate, because manganese contributes strength and toughness and the specification will not leave that to chance.

Silicon works the same way. A516 sets a range with a floor, since the steel must be fully killed. A36 sets only a ceiling.

Carbon is the surprise. A516 Grade 70 actually permits slightly more carbon than A36 at comparable thicknesses. Higher carbon is what delivers the tensile strength, and A516 compensates for its effect on weldability by controlling everything else tightly. If you assumed the pressure vessel plate must be the lower carbon one, the table says otherwise.

Steelmaking Practice and Traceability

A516 requires fully killed steel at every thickness. A36 requires killed steel only on plate above 40 mm, and below that the producer may use whichever practice it prefers.

That single line explains most of the behavioural difference between the two. Semi-killed steel retains more dissolved gas, shows more variation through the plate thickness, and is less predictable in the areas a pressure vessel cares about, namely internal soundness and resistance to brittle fracture.

Traceability differs in the same way. A516 plate is supplied with full heat traceability and hard stamped identification as a matter of course. A36 is often supplied to a general certificate without the same level of individual plate identification, which is adequate for structural steel and inadequate for a code vessel.

Notch Toughness and Impact Testing

A516 was written with notch toughness as a design objective. The fine grain requirement exists specifically to resist brittle fracture, and Charpy V-notch testing is available as a supplementary requirement, commonly specified at 0 °C, −20 °C or −46 °C depending on the minimum design metal temperature.

A36 has no fine grain requirement and no impact testing provision within the specification. It is not that A36 is brittle. It is that its toughness is neither guaranteed nor verified, so nobody can certify how it will behave at low temperature.

Both grades leave impact testing optional in the sense that you must ask for it, but only A516 has the underlying metallurgy to reliably meet a demanding requirement when you do.

Can A36 Be Used for a Pressure Vessel?

Inspection of a fabricated pressure vessel for code compliance

Most articles answer this with a flat no. That is a reasonable rule of thumb but it is not what the code says, and the real answer is more useful.

Under ASME Section VIII Division 1, SA-36 plate is permitted for pressure parts, subject to restrictions set out in UCS-6. The main ones are:

  • Thickness is limited to 5/8 in (16 mm). Above that, SA-36 may not be used for pressure parts.
  • Not permitted in vessels containing lethal substances. UCS-6 excludes SA-36, along with SA-283 grades, from lethal service.
  • Not permitted for unfired steam boilers.

So a small, low-pressure, non-lethal vessel in thin plate can legitimately use SA-36 within Division 1. Beyond those boundaries it cannot, and that covers the overwhelming majority of real vessels, which is why the blanket “no” persists as practical advice.

Three points before anyone treats this as permission:

The certificate must say SA-36, not A36. Only the ASME-adopted specification is acceptable for code construction. This is the same relationship that exists between ASTM A516 and ASME SA516, where the steel is identical and only the certified designation decides whether an inspector accepts it.

The restrictions are cumulative. Meeting the thickness limit does not help if the service is lethal.

Read the current code edition. UCS-6 has been revised over the years, and the clause numbering and limits should be confirmed against the edition your project works to rather than taken from any article, including this one.

If cost is what is pushing you toward A36 for a pressure application, the better answer is usually a lower cost PVQ plate rather than a structural one. The comparison with A285 Grade C covers where a lighter pressure vessel specification is sufficient.

Can A516 Grade 70 Be Used for Structural Work?

Yes, without restriction. A516 Grade 70 exceeds A36 on tensile strength and matches it on yield, and nothing in structural design prevents using a plate certified to a more demanding specification.

Whether you should is a different question. You would be paying 10 to 20% more for controlled steelmaking, tighter impurity limits and traceability that a beam or base plate makes no use of. In most cases that is wasted money.

Where it does make sense is consolidation. On a fabrication project already buying a516 gr 70 plate in quantity for vessels, using the same plate for supports, saddles and brackets can simplify stock control, reduce offcut waste and remove the risk of the wrong plate reaching the wrong part of the job. That last point is worth real money on a shop floor.

Weldability and Fabrication

Welding carbon steel plate in an industrial fabrication shop

Both grades weld well, and both are commonly joined with low-hydrogen consumables such as E7018.

A36 is the easier of the two. Its lower manganese and generally lower carbon equivalent mean preheat is often unnecessary on thinner sections, and it tolerates a wider range of procedures without trouble.

A516 Grade 70 needs more discipline as thickness rises. Carbon equivalent typically runs 0.43 to 0.45, so low-hydrogen practice matters throughout, the plate should be dry and free of scale, and preheat becomes important above roughly 40 mm. Post-weld heat treatment may also be required depending on thickness and service, since ASME Section VIII sets PWHT rules that structural work simply does not have.

The fabrication difference is therefore less about difficulty and more about governance. A516 work carries qualified welding procedures, qualified welders and documented inspection. A36 structural work carries its own quality requirements under AWS D1.1, but they are a different framework with different objectives.

Cost and Availability

A36 is the cheapest carbon steel plate in general circulation and the most widely available in thin gauges. It is stocked almost everywhere.

A516 Grade 70 typically runs 10 to 20% higher per tonne. That premium buys the controlled steelmaking, the testing and the certification, not extra strength alone. It is also very widely stocked, since it is the most commonly specified pressure vessel plate in the world, and it is available in a broader thickness range at the heavy end.

The premium is easy to justify on a vessel and hard to justify on a frame, which is the whole basis of the decision.

Applications

Structural steel frame built from A36 carbon steel plate

ASTM A36 is used for building frames and structural columns, bridge components such as plate girders and gusset plates, machinery bases and equipment supports, crane and lifting structures, transmission towers, general fabrication, and base plates and embeds.

ASTM A516 Grade 70 is used for pressure vessels and reactors in refinery and petrochemical service, industrial boilers, storage tanks to API 650 and API 620, heat exchanger shells and channels, columns and drums, LPG and ammonia storage, and deaerators and feedwater heaters in power plants.

Documentation Differences

Mill test certificate supplied with carbon steel plate

What you should ask for changes with the specification.

For A36, a mill test certificate covering chemistry and tensile results is normally sufficient for structural work.

For A516 Grade 70, ask for more:

  1. EN 10204 Type 3.1 certificate as a minimum, showing heat number, chemical analysis, tensile results and plate dimensions. Type 3.2 where third party inspection is required.
  2. Delivery condition stated, as-rolled or normalized, with normalizing confirmed on the certificate where specified.
  3. Charpy impact results where the design temperature calls for them, with the test temperature and energy recorded.
  4. Ultrasonic examination where internal soundness matters, typically to ASTM A578.
  5. SA-516 named on the certificate if the vessel is code stamped.

Frequently Asked Questions

What is the main difference between A36 and A516 Grade 70?

A36 is a structural steel for buildings, bridges and machinery, while A516 Grade 70 is pressure vessel quality plate for welded vessels and boilers. The difference goes beyond strength to steelmaking control, since A516 requires fully killed fine grain steel with tighter impurity limits, full traceability and access to impact and ultrasonic testing that A36 does not offer.

Can I use A36 plate for a pressure vessel?

In limited circumstances yes, but rarely in practice. ASME Section VIII Division 1 permits SA-36 for pressure parts up to 5/8 in (16 mm) thick, excluding lethal service and unfired steam boilers. Beyond those limits it is not permitted, and the material must be certified as SA-36 rather than A36. For most vessels the practical answer is to use A516.

Is A516 Grade 70 stronger than A36?

On tensile strength yes, at 485 to 620 MPa against 400 to 550 MPa, a difference of about 21% at the minimum. On yield strength the two are close, at 260 MPa against 250 MPa. The tensile gap matters most because ASME derives allowable stress from minimum tensile strength.

Does A516 Grade 70 have more carbon than A36?

Slightly more at comparable thicknesses, which surprises many buyers. The carbon is what produces the higher tensile strength, and A516 offsets its effect on weldability by controlling manganese, silicon, phosphorus and sulphur far more tightly and by mandating killed fine grain steel.

Can I use A516 Grade 70 for structural work?

Yes, and it will exceed A36 in every mechanical property. It usually costs more than the application justifies, so it is worth doing only where consolidating to one plate grade simplifies purchasing or reduces the risk of the wrong material reaching the wrong component.

What does PVQ plate mean?

Pressure vessel quality. It describes plate produced to a specification written for pressure containment, which brings controlled steelmaking practice, tighter chemistry, full heat traceability and an established framework of optional testing. A516, A285, A515 and A537 are all PVQ specifications. A36 is not.

Which is more ductile, A36 or A516 Grade 70?

A36, on both gauge lengths. It requires 20% elongation over 200 mm and 23% over 50 mm, against 17% and 21% for A516 Grade 70. That extra ductility makes A36 easier to form, though it comes with lower tensile strength.

Do A36 and A516 Grade 70 weld differently?

Both weld well with low-hydrogen consumables, but A516 Grade 70 needs more care as thickness increases because its carbon equivalent is higher, making preheat important above roughly 40 mm. The bigger difference is procedural, since pressure vessel work brings qualified welding procedures, documented inspection and potential post-weld heat treatment requirements that structural work does not.

In Short

A36 and A516 Grade 70 are built for different jobs, and the specifications reflect that rather than simply ranking one above the other. A36 sets outer limits and leaves the rest to the mill. A516 controls the steelmaking, the impurities, the grain structure and the traceability, because a vessel failure and a beam failure are not comparable events.

The strength gap is narrower than most people expect, particularly on yield. What you are really buying with A516 is certainty, and the certificate that proves it.

For a vessel, boiler or tank, specify A516. For a frame, base or structural member, specify A36. The one case worth checking properly is a small thin-walled vessel, where the code permits SA-36 within limits that are much tighter than most projects can live with.

Found this useful? Share it.

Popular articles