A516 Grade 70 and A537 Class 1 carry the same tensile range, 485 to 620 MPa. That coincidence sends a lot of buyers down the wrong path, because the two plates are not interchangeable and the specification titles explain why. A516 is written for carbon steel in moderate and lower temperature service. A537 is written for heat-treated carbon-manganese-silicon steel, and every plate supplied under it has been through a mandatory heat treatment that A516 leaves optional.
A537 splits into classes according to that treatment. Class 1 is normalized. Class 2 is quenched and tempered, which lifts it well above both of the others on strength.
The three plates differ on heat treatment, strength, ductility, chemistry, toughness and welding behaviour, and each of those is covered below. One point deserves attention early, because supplier pages rarely mention it. The higher yield strength of A537 Class 1 buys you no reduction in wall thickness under ASME Section VIII Division 1, which changes the entire cost argument for choosing it.
A516 Grade 70 vs A537 Class 1 vs Class 2: Property Comparison
Values shown are for plate 65 mm and under, where all three grades are most commonly supplied.
| A516 Grade 70 | A537 Class 1 | A537 Class 2> | |
|---|---|---|---|
| Specification type | Carbon steel | Heat-treated C-Mn-Si steel | Heat-treated C-Mn-Si steel |
| Heat treatment | Optional below 40 mm | Normalized, mandatory | Quenched and tempered, mandatory |
| Tensile strength | 485–620 MPa | 485–620 MPa | 550–690 MPa |
| Yield strength, minimum | 260 MPa | 345 MPa | 415 MPa |
| Elongation in 50 mm, min | 21% | 22% | 22% |
| Elongation in 200 mm, min | 17% | 18% | No requirement |
| Carbon, maximum | 0.27 to 0.31% | 0.24% | 0.24% |
| Allowable stress, ASME VIII-1 | 20.0 ksi | 20.0 ksi | 22.9 ksi |
| Relative cost | Lowest | Higher | Highest |
Heat Treatment Difference: As-Rolled, Normalized and Quenched and Tempered
A516 permits plate to be supplied as-rolled. Below 40 mm that is the default, and normalizing happens only if you write it on the purchase order. Above 40 mm the plate is normalized as standard, which is one of several conditions covered in the mechanical properties of A516 Grade 70 plate.
A537 has no as-rolled option at all. The specification title contains the words heat-treated, and every plate is treated before it ships.
Class 1 is normalized. The plate is heated to around 900 °C and cooled in still air. This refines the grain structure and evens out the composition, producing uniform properties and good toughness.
Class 2 is quenched and tempered. The plate is heated, then cooled rapidly in water, which creates a hard and brittle structure. It is then reheated to a tempering temperature of at least 595 °C, which restores toughness while keeping most of the strength gained during quenching.
Quench and temper is a more controlled and more expensive route than normalizing, and it produces a finer, tougher structure at higher strength. That is the whole reason Class 2 exists.
Mechanical Properties Comparison: Tensile and Yield Strength
A537 Class 1 and A516 Grade 70 share the same tensile range, so tensile strength tells you nothing useful when comparing them. Yield strength is where they part company.
| Grade | Minimum yield | Increase over A516 Gr 70 |
|---|---|---|
| A516 Grade 70 | 260 MPa | Baseline |
| A537 Class 1 | 345 MPa | 33% higher |
| A537 Class 2 | 415 MPa | 60% higher |
A537 Class 1 delivers a third more yield strength at the same tensile strength. In practical terms the plate stays elastic under much higher stress before it takes a permanent set, and the gap between yield and tensile narrows, which is characteristic of a heat-treated steel.
Class 2 goes further and lifts tensile strength as well, reaching 550 to 690 MPa. It is the strongest of the three by a clear margin.
Why A537 Class 1 Does Not Reduce Wall Thickness Under ASME Section VIII
Here is the point that changes how you should think about A537 Class 1, and it appears on almost no supplier page.
ASME Section VIII Division 1 sets allowable stress as the lower of two figures: minimum tensile strength divided by 3.5, or two thirds of minimum yield strength. Run both grades through it.
| Grade | Tensile ÷ 3.5 | Two thirds of yield | Allowable stress |
|---|---|---|---|
| A516 Grade 70 | 20.0 ksi | 25.3 ksi | 20.0 ksi |
| A537 Class 1 | 20.0 ksi | 33.3 ksi | 20.0 ksi |
| A537 Class 2 | 22.9 ksi | 40.0 ksi | 22.9 ksi |
Because both grades share the same 70 ksi minimum tensile strength, and because tensile governs in Division 1, A537 Class 1 and A516 Grade 70 carry the same allowable stress. The extra yield strength is real, but Division 1 does not credit it. Your vessel wall comes out the same thickness on both.
So when you pay more for A537 Class 1, you are not buying a thinner vessel. You are buying guaranteed normalized condition, better toughness, lower carbon and easier welding. Those can be excellent reasons. Reduced steel tonnage is not one of them.
Class 2 is different. Its higher tensile strength does raise allowable stress to 22.9 ksi, roughly 15% above A516 Grade 70, so it genuinely reduces wall thickness.
Two caveats. Division 2 uses different design rules and gives more weight to yield strength, so the picture changes there. And allowable stress values should always be read from the current ASME Section II Part D tables for your code edition rather than calculated by hand.
How Plate Thickness Affects A537 Class 1 and Class 2 Properties
A516 Grade 70 holds the same strength requirements at every thickness. A537 does not, and this trips people up on heavy sections.
A537 Class 1
| Thickness | Tensile | Yield, minimum |
|---|---|---|
| Up to 65 mm | 485–620 MPa | 345 MPa |
| Over 65 to 100 mm | 450–585 MPa | 310 MPa |
| Over 100 to 150 mm | 450–585 MPa | 310 MPa |
A537 Class 2
| Thickness | Tensile | Yield, minimum |
|---|---|---|
| Up to 65 mm | 550–690 MPa | 415 MPa |
| Over 65 to 100 mm | 515–655 MPa | 380 MPa |
| Over 100 to 150 mm | 485–620 MPa | 315 MPa |
The reason is physical. Heat treatment works from the surface inward, so a thick plate cools more slowly at its core and cannot reach the same properties throughout. The specification is honest about that limitation and reduces the requirement accordingly.
The consequence is worth noting. At 120 mm, A537 Class 1 has a minimum yield of 310 MPa against 260 MPa for A516 Grade 70, so the advantage narrows considerably. And A537 Class 2 at 120 mm has fallen to a 485 to 620 MPa tensile range, exactly matching A516 Grade 70. If you specified Class 2 on a heavy section expecting a strength benefit, check the table before you commit.
Elongation and Ductility Comparison
The strength gain does not cost ductility here, which surprises people used to the trade-off within the A516 family.
| Grade | Elongation in 50 mm | Elongation in 200 mm |
|---|---|---|
| A516 Grade 70 | 21% | 17% |
| A537 Class 1 | 22% | 18% |
| A537 Class 2 | 22% | Not required |
A537 Class 1 is both stronger and marginally more ductile than A516 Grade 70. That is possible because its strength comes from heat treatment and manganese rather than carbon, and carbon is what usually destroys ductility.
Note the last cell. A537 Class 2 has no elongation requirement over a 200 mm gauge length at all, so ductility is verified only over 50 mm. If your specification or client demands an 8 inch elongation figure, Class 2 will not provide one.
Both A537 classes cold form well. Mill guidance calls for grinding away shear burrs, thermal cutting heat-affected zones and sharp corners near the bend axis before forming, which matters more on heat-treated plate than on as-rolled material.
Chemical Composition Comparison
| Element | A516 Grade 70 | A537 Class 1 and 2 |
|---|---|---|
| Carbon | 0.27 to 0.31% max, by thickness | 0.24% max |
| Manganese | 0.85–1.20% | 0.70–1.35%, up to 1.60% permitted |
| Silicon | 0.15–0.40% | 0.15–0.50% |
| Phosphorus | 0.025% max | 0.035% max |
| Sulphur | 0.025% max | 0.035% max |
| Nickel | Not specified | 0.25% max, up to 0.50% permitted |
A537 reaches higher strength on less carbon, not more. It substitutes manganese, silicon and heat treatment instead. That combination is the standard metallurgical route to strength without sacrificing weldability or toughness, and it is why A537 performs so well in the cold.
The manganese and nickel allowances come with a condition. Manganese may rise to 1.60% and nickel to 0.50% only if the heat analysis carbon equivalent stays at or below 0.57. The specification lets the mill trade one element against another as long as the weldability index holds.
One honest point in A516’s favour. A516 Grade 70 has tighter phosphorus and sulphur limits, 0.025% against 0.035%. On raw impurity control the carbon steel is the cleaner specification, which is worth remembering if inclusion content matters to your application.
Impact Toughness and Low Temperature Service
Both specifications are aimed at moderate and lower temperature service, and Charpy V-notch testing is a supplementary requirement in both. Neither is impact tested unless you ask.
The difference is how much toughness is available when you do ask. A537 has three advantages built in: guaranteed heat treatment, lower carbon, and higher manganese. Class 2 adds the finer structure that quenching and tempering produces.
The practical ranking for cold service runs from as-rolled A516 Grade 70 at the bottom, through normalized A516 Grade 70N, then A537 Class 1, to A537 Class 2 at the top.
This is where A537 earns its price. For LPG spheres, ammonia storage, offshore equipment and API 620 low-temperature tanks, the toughness margin is the reason to specify it, not the strength.
Weldability and Fabrication Differences
All three grades weld well. Low-hydrogen consumables, dry plate and appropriate preheat apply throughout.
A537 has a genuine advantage on carbon equivalent. Its carbon ceiling of 0.24% is well below the 0.28 to 0.31% that A516 Grade 70 permits on thicker plate, and the specification caps carbon equivalent at 0.57 when the manganese and nickel allowances are used. Lower carbon equivalent means less risk of hydrogen cracking in the heat-affected zone.
Class 2 needs more care during welding regardless. Its properties come from a controlled quench and temper cycle, and excessive heat input during welding can soften the heat-affected zone and undo locally what the heat treatment achieved. Heat input limits should be set in the welding procedure rather than left to the welder.
Post-Weld Heat Treatment Limits for A537 Class 2
This deserves its own warning because it can quietly ruin a vessel.
A537 Class 2 is tempered at a minimum of 595 °C. Post-weld heat treatment for carbon steel is commonly performed in the region of 595 to 620 °C. Those two ranges overlap.
If PWHT temperature approaches or exceeds the original tempering temperature, the plate is effectively being re-tempered, and its certified mechanical properties may no longer apply. The vessel could leave the shop weaker than the design assumed, with a certificate that says otherwise.
Where a Class 2 vessel will be stress relieved, do two things. Agree the PWHT temperature and holding time with the plate mill before ordering, and consider Supplementary Requirement S3, simulated post-weld heat treatment of mechanical test coupons, so the certified properties reflect the plate as it will exist after fabrication rather than as it left the mill.
A516 Grade 70 and A537 Class 1 do not carry this risk in the same way, since normalized material is far less sensitive to a subsequent stress relief cycle.
Cost and Availability Comparison
A516 Grade 70 is the cheapest and by a wide margin the most widely stocked pressure vessel plate in the world. It is available in more thicknesses, more sizes and from more mills than the other two combined.
A537 Class 1 costs more because normalizing is a mandatory extra process step. Stock is reasonable but thinner than A516.
A537 Class 2 costs the most, since quenching and tempering is a more demanding operation with tighter control. It is often a mill order rather than a stock item, so lead time should be checked early in a project.
The commercial logic follows the allowable stress table above. Paying more for Class 1 does not reduce your steel tonnage under Division 1, so it only makes sense when you need the toughness or the guaranteed normalized condition. Class 2 does reduce tonnage, so on a large high-pressure vessel the extra plate cost can be partly recovered in weight, welding and handling.
Applications: Where Each Grade Is Used
A516 Grade 70 is the default for general pressure vessel work: reactors and vessels in refineries and petrochemical plants, boiler drums, heat exchanger shells and tubesheets, and process tanks. When a project calls for astm a516 grade 70 plate, it is usually because the duty is well within reach of a standard carbon steel and there is no reason to pay for heat treatment.
A537 Class 1 suits vessels and tanks that need dependable toughness with uniform properties, including API 650 and API 620 storage tanks, low-temperature process vessels, and equipment where a guaranteed normalized condition is part of the client specification.
A537 Class 2 is for the demanding end: high-pressure vessels where wall thickness must be minimised, LPG and LNG-adjacent storage spheres, offshore and marine structures, and cold-service equipment with strict Charpy requirements.
Which Grade to Choose: A516 Grade 70, A537 Class 1 or Class 2
Work down this list and stop at the first line that fits.
- Standard pressure vessel, ambient or moderate temperature, cost matters. A516 Grade 70.
- Cold service with impact requirements you are confident A516 Grade 70N can meet. Normalized A516 Grade 70, which is cheaper than either A537 class.
- Client specification demands guaranteed normalized plate, or Charpy requirements A516 struggles with. A537 Class 1.
- High pressure where wall thickness and vessel weight drive the cost. A537 Class 2, since it is the only one of the three that raises allowable stress.
- Severe low temperature with demanding impact energy. A537 Class 2.
- Plate over 100 mm. Recheck the thickness tables. The A537 advantage narrows sharply and may not justify the price
Frequently Asked Questions
Is A537 Class 1 stronger than A516 Grade 70?
On yield strength yes, by about 33%, at 345 MPa against 260 MPa. On tensile strength the two are identical at 485 to 620 MPa. Because ASME Section VIII Division 1 sets allowable stress from tensile strength, both grades carry the same 20.0 ksi allowable stress and produce the same wall thickness.
What is the difference between A537 Class 1 and Class 2?
Heat treatment. Class 1 is normalized, meaning heated and air-cooled. Class 2 is quenched and tempered, meaning rapidly cooled then reheated to at least 595 °C. Class 2 comes out considerably stronger at 550 to 690 MPa tensile and 415 MPa minimum yield, with better low-temperature toughness.
Can A537 Class 1 replace A516 Grade 70?
Technically yes, since it meets or exceeds every A516 Grade 70 mechanical requirement. Whether it is worth doing is another question. Under Division 1 you gain no thickness reduction, so you are paying extra for toughness and guaranteed normalizing rather than for less steel. Any substitution also needs written approval from the design engineer and a check on welding procedure qualification.
Why does A537 have lower carbon than A516 Grade 70?
Because its strength comes from heat treatment and manganese instead. A537 caps carbon at 0.24% while A516 Grade 70 allows up to 0.31% on thick plate. Lower carbon means a lower carbon equivalent, which improves weldability and toughness, and the heat treatment makes up the strength.
Does A537 need impact testing?
Only if you specify it, exactly as with A516. Charpy V-notch testing is a supplementary requirement in both specifications. The difference is capability rather than default, since A537 will meet demanding low-temperature requirements far more reliably thanks to its heat treatment and lower carbon.
Do A537 properties change with plate thickness?
Yes, and significantly. Class 1 minimum yield drops from 345 MPa to 310 MPa above 65 mm. Class 2 drops from 415 MPa to 380 MPa above 65 mm and to 315 MPa above 100 mm, with tensile falling to 485 to 620 MPa. A516 Grade 70 holds the same requirements at every thickness, so the gap narrows as plate gets heavier.
What should I watch out for when stress relieving A537 Class 2?
The tempering temperature. Class 2 is tempered at a minimum of 595 °C, and typical PWHT for carbon steel runs 595 to 620 °C, so the two overlap. Stress relieving at or above the tempering temperature can reduce the certified properties. Agree the PWHT cycle with the mill before ordering and consider specifying simulated post-weld heat treatment of the test coupons.
Which grade is best for LPG and low temperature storage tanks?
A537 Class 2 for the most demanding duty, with Class 1 a common choice for API 650 and API 620 tanks. Both were written with notch toughness in mind. Normalized A516 Grade 70 handles many low-temperature applications successfully and at lower cost, so it is worth checking whether it meets your Charpy requirement before moving up.
Key Takeaways
A516 Grade 70 and A537 Class 1 look alike on a tensile table and behave differently everywhere else. A537 Class 1 gives you a third more yield strength, mandatory normalizing, lower carbon and better toughness, but no reduction in wall thickness under Division 1. A537 Class 2 is the genuine step up, raising both tensile strength and allowable stress, at the highest price and with real constraints around welding heat input and post-weld heat treatment.
The sensible approach is to treat A516 Grade 70 as the starting point and require a specific reason to move away from it. If that reason is toughness, Class 1 is the logical step. If it is pressure and vessel weight, Class 2 is the only one of the three that will actually thin the wall. And on plate above 100 mm, recheck the thickness tables before assuming any upgrade is buying what you think it is.