A516 Grade 70 can be supplied in several different conditions, and the condition matters as much as the grade. Two plates with identical tensile results can behave very differently in cold service depending on whether they were heat treated and how.
The specification handles this in a way that surprises people. Heat treatment is mandatory above a certain thickness, optional below it, and triggered automatically by something apparently unrelated: ordering impact testing. Get any of these wrong on the purchase order and the plate that arrives may meet every number on the certificate while still being unsuitable for the job.
This blog explains each heat treatment condition A516 Grade 70 can be supplied in, when normalizing is required and when it is a choice, how stress relief differs from normalizing, what accelerated cooling adds, and how post-weld heat treatment affects the properties you certified.
Why Heat Treatment Matters for This Grade
A516 exists because of notch toughness. The specification describes itself as covering plates for welded pressure vessels where improved notch toughness is important, and every requirement in it supports that.
Two of those requirements are built into steelmaking. The steel must be killed, so it solidifies without gas porosity, and it must meet a fine austenitic grain size requirement, because fine grain is what stops a small crack running through the plate.
Heat treatment is the third lever. Rolling leaves the plate with a structure that varies through its thickness, particularly on heavy sections. Reheating and controlled cooling resets that structure, making it finer and more uniform. The tensile figures barely move. The toughness moves a great deal.
That is the key to understanding everything below. Heat treatment on A516 Grade 70 is about toughness, not strength.
The Supply Conditions Available
A516 Grade 70 can be supplied in any of the following.
| Condition | What it means |
|---|---|
| As-rolled | No heat treatment after rolling |
| Normalized | Reheated and cooled in still air |
| Stress relieved | Heated to relieve residual stress, then slowly cooled |
| Normalized and stress relieved | Both operations, in that order |
| Accelerated cooled and tempered | Cooled faster than air, then tempered |
The first four are the common ones and appear routinely on mill certificates. The fifth is permitted by the specification but used less often, and is covered further down.
Whichever applies, the condition is recorded on the mill test certificate. It should always be checked against what was ordered
As-Rolled Condition
As-rolled means the plate went from the rolling mill to the cooling bed and nothing further was done to it.
This is the normal supply condition for plate of 40 mm and under. It is the cheapest route, because no furnace time is involved, and for a great many vessels it is entirely adequate.
Where as-rolled plate falls short is low-temperature toughness. The structure is less uniform than a heat treated plate, particularly through the thickness, so its resistance to brittle fracture is lower and less predictable. For an ambient-temperature vessel that rarely matters. For anything running cold, it does.
Normalizing
Normalizing means reheating the plate above its transformation temperature, typically in the region of 900 °C, holding it, then cooling it in still air.
What happens metallurgically is grain refinement. The existing structure transforms as the plate is heated, and when it cools in air it forms again as smaller, more uniform grains. Composition differences left over from rolling also even out.
The result is a plate with much the same strength and noticeably better toughness, especially in the cold. This is why normalized plate is the standard choice for cold service and why the designation Gr 70N exists.
Normalizing costs money. It is a separate furnace operation with its own energy, handling and time, and it often adds lead time as well. That is why the specification does not require it on every plate.
When Normalizing Is Mandatory
There are two rules, and the second one is missed constantly.
Plate over 40 mm must be normalized. This is not optional and is not something you specify. Heavy plate cools slowly and unevenly during rolling, and normalizing is the only way to give it a uniform structure through the thickness. The cost is already built into the price of heavy plate.
Impact testing on thin plate brings normalizing with it. Where notch toughness testing is required on plate of 40 mm and under, the specification requires the plate to be normalized unless the purchaser specifies otherwise. So a buyer who orders Charpy testing on 25 mm plate receives normalized plate automatically, whether or not they asked for it.
That second rule has two practical effects. It means you do not need to write both requirements separately, since ordering the test brings the heat treatment. And it means the cost of impact testing on thin plate is higher than the test alone, because normalizing arrives with it.
Below 40 mm, with no impact testing required, plate is supplied as-rolled unless you write normalized or Gr 70N on the order.
Stress Relief
Stress relief is often confused with normalizing. They are different operations with different purposes.
Normalizing changes the structure of the steel to improve its properties. It is done at high temperature, above the transformation point.
Stress relief removes internal stress without changing the structure. It is done at a lower temperature, below the transformation point, and the plate is cooled slowly rather than in still air.
Residual stress builds up in steel during rolling, cutting, forming and especially welding. Left in place it can cause distortion during machining, contribute to cracking, and make a vessel more vulnerable in service. Heating the steel allows those stresses to relax.
Stress relief can be applied at the mill, as a delivery condition on the plate, or after fabrication as post-weld heat treatment on the finished vessel. The second is far more common, since welding introduces more stress than rolling does.
Accelerated Cooling and Tempering
This route is permitted by the specification and rarely discussed.
Where the purchaser approves it, plate may be cooled faster than still air to improve toughness, provided it is then tempered in the range 595 to 705 °C.
The logic is the same as any quench and temper process. Faster cooling produces a finer, tougher structure than air cooling can achieve, but it also leaves the steel harder and more brittle than wanted. Tempering afterwards restores ductility while keeping most of the toughness gained.
Two conditions apply. It requires purchaser approval, so it cannot be done unilaterally by the mill. And the tempering step is mandatory, not optional.
In practice most cold-service work uses normalizing, which is simpler and widely available. Accelerated cooling is worth knowing about when a demanding toughness requirement is proving difficult to meet by normalizing alone.
Simulated Post-Weld Heat Treatment
This is the heat treatment issue that causes the most trouble on real projects, and it concerns the test coupons rather than the plate.
When a vessel is stress relieved after welding, the plate spends hours at high temperature. That thermal cycle slightly reduces its strength. So the vessel in service is marginally weaker than the plate was when the mill tested it, and the certificate no longer describes the material as it now exists.
The specification provides for this. Supplementary Requirement S3, simulated post-weld heat treatment of mechanical test coupons, asks the mill to put the test coupons through the same thermal cycle the vessel will experience before running the tension test. The certified properties then reflect the plate as it will be in the finished vessel.
Two things to remember. Like all supplementary requirements, S3 applies only if it is written on the purchase order. And the mill needs to know the PWHT cycle you intend to use, so it has to be agreed at enquiry stage rather than added later.
For most ambient-service vessels the difference is small enough to ignore. Where the design has little margin, or where a client specification demands it, S3 is the correct answer.
How Heat Treatment Affects the Properties
The tensile requirements do not change with delivery condition. A normalized plate and an as-rolled plate must both meet 485 to 620 MPa tensile and 260 MPa minimum yield.
What changes is toughness, and the practical ranking runs like this.
| Condition | Relative low-temperature toughness |
|---|---|
| As-rolled | Baseline |
| Normalized | Noticeably better |
| Accelerated cooled and tempered | Better still |
Hardness moves slightly with condition too, with normalized plate typically testing a little higher than as-rolled, though the specification sets no hardness requirement either way.
The point worth carrying away is that two certificates showing near-identical tensile results can represent plates that behave very differently at low temperature. The delivery condition line is as important as the test figures beside it.
What Appears on the Certificate
The mill test certificate records the delivery condition, and it should be read alongside the thickness and the test results.
Four checks are worth making.
Does the condition match the order? As-rolled supplied where normalized was specified is a genuine rejection point, and no amount of good tensile data fixes it.
Is it consistent with the thickness? Plate over 40 mm should show normalized. If it does not, question it.
Is it consistent with the testing? A certificate reporting impact values on plate of 40 mm or under should normally also show the normalized condition, because the specification links the two.
Was normalizing confirmed with detail? Many mills state the temperature and that the plate was air cooled. Where a client specification requires evidence of the heat treatment, this is what satisfies it.
What to Specify on Your Order
Heat treatment problems are almost always ordering problems. State the following.
- Delivery condition, as-rolled, normalized, stress relieved, or normalized and stress relieved.
- The Gr 70N designation where normalized plate is required below 40 mm.
- Impact testing with the temperature, energy and orientation, remembering that on thin plate this brings normalizing with it.
- Simulated PWHT under S3, together with the thermal cycle you intend to apply, where the vessel will be stress relieved and the design margin is tight.
- Any client or project requirement for evidence of heat treatment on the certificate.
None of these can be added economically after the plate is rolled. Impact testing in particular may require material from a new heat if the coupons no longer exist.
Frequently Asked Questions
Does A516 Grade 70 need heat treatment?
It depends on thickness and on what you are testing for. Plate over 40 mm must be normalized. Plate of 40 mm and under is normally supplied as-rolled, unless you order normalizing or require notch toughness testing, which brings normalizing with it under the specification.
What does normalized mean for A516 Grade 70?
The plate has been reheated to around 900 °C, held, then cooled in still air. This refines the grain structure and evens out composition differences left from rolling, producing a plate with similar strength but noticeably better toughness at low temperature. It is often designated Gr 70N.
What is the difference between normalizing and stress relief?
Normalizing is a high-temperature treatment that changes the steel’s structure to improve its properties, followed by air cooling. Stress relief is a lower-temperature treatment that relaxes internal stresses without changing the structure, followed by slow cooling. They solve different problems and are sometimes both applied.
Why is plate over 40 mm always normalized?
Because thick plate cools slowly and unevenly after rolling, leaving a structure that varies through its thickness. Normalizing is the only practical way to make that structure uniform, so the specification makes it mandatory rather than optional above 40 mm.
Does ordering impact testing change the delivery condition?
Yes, on thin plate. Where notch toughness tests are required on plate of 40 mm and under, the standard requires the plate to be normalized unless the purchaser states otherwise. This means the cost of impact testing on thin plate includes a normalizing cycle.
Does post-weld heat treatment reduce the properties?
Slightly. The plate spends hours at elevated temperature during stress relief, which reduces strength a little. Where that matters, specify Supplementary Requirement S3, simulated post-weld heat treatment of mechanical test coupons, so the certified properties reflect the plate as it will exist in the finished vessel.
Can A516 Grade 70 be quenched and tempered?
The specification permits cooling faster than still air, with purchaser approval, provided the plate is afterwards tempered between 595 and 705 °C. It is used where a demanding toughness requirement cannot comfortably be met by normalizing. Most cold-service work uses normalizing, which is simpler and more widely available.
Does heat treatment change the tensile strength?
Not in terms of the requirement. Every condition must meet the same 485 to 620 MPa tensile range and 260 MPa minimum yield. What heat treatment changes is toughness, which is why two plates with almost identical tensile results can perform very differently in cold service.
What This Means in Practice
Heat treatment on A516 Grade 70 is a toughness decision, not a strength decision. The tensile requirements are the same whichever condition the plate is supplied in.
Three rules cover nearly every situation. Plate over 40 mm arrives normalized and you do not need to ask. Plate of 40 mm and under arrives as-rolled unless you ask for normalizing. And ordering impact testing on thin plate brings normalizing with it automatically.
The two things worth deciding early are whether your service temperature genuinely needs normalized plate, since specifying it out of caution adds cost that the design may not require, and whether the vessel will be stress relieved after welding in a way that makes simulated PWHT worth specifying.
Both are enquiry-stage decisions. Neither can be added economically once the plate has been rolled.