ASTM A516 is the specification for carbon steel plate used in welded pressure vessels operating at moderate and lower temperatures. It comes in four grades, and three of them account for almost all commercial demand: Grade 60, Grade 65 and Grade 70. All three share the same specification, the same testing rules and the same fine-grain requirement. What separates them is strength.
The grade number tells you the minimum tensile strength in ksi, so Grade 70 is stronger than Grade 65, which is stronger than Grade 60. That extra strength is bought with extra carbon, and carbon is where the trade-offs begin. More carbon lifts strength but reduces ductility, makes welding more demanding, and slightly lowers notch toughness. Choosing between the grades is really a decision about which of those things matters most in your vessel.
This guide compares all three side by side on strength, elongation, chemistry, toughness and allowable stress. It then looks at the practical consequences: how grade choice changes wall thickness and cost, how it affects welding, where each grade is typically used, and which one is the sensible default for most projects.
A516 Grade 60 vs 65 vs 70 at a Glance
| Property | Grade 60 | Grade 65 | Grade 70 |
|---|---|---|---|
| Tensile strength (MPa) | 415–550 | 450–585 | 485–620 |
| Tensile strength (ksi) | 60–80 | 65–85 | 70–90 |
| Yield strength min (MPa) | 220 | 240 | 260 |
| Yield strength min (ksi) | 32 | 35 | 38 |
| Elongation in 200 mm, min | 21% | 19% | 17% |
| Elongation in 50 mm, min | 25% | 23% | 21% |
| Allowable stress, ASME VIII-1 (ksi) | 17.1 | 18.6 | 20.0 |
| Relative availability | Good | Limited | Excellent |
Read the table from left to right and the pattern is immediate. Every step up in grade adds roughly 35 MPa of tensile strength and 20 MPa of yield strength, and costs you two percentage points of elongation.
Difference in Strength
Strength is the whole reason the grades exist, and it shows up in two numbers.
Tensile strength is the maximum stress the plate carries before it starts to break. Note that all three grades specify a range rather than a floor. Grade 60 must test between 415 and 550 MPa, and a plate testing at 570 MPa fails the specification even though it is stronger. The ceiling exists because a pressure vessel is designed to deform visibly before it ruptures, and steel that is too strong is usually too brittle to give that warning.
Yield strength is the point where the plate stops springing back and starts to deform permanently. Only a minimum is given, so plates routinely test above it.
The practical gap between Grade 60 and Grade 70 is about 17% on both measures. That sounds modest, but on a large vessel it translates directly into plate thickness and tonnage.
Difference in Ductility
Ductility is how far the steel stretches before it fractures, reported as elongation over a fixed gauge length.
| Grade | Elongation in 200 mm | Elongation in 50 mm |
|---|---|---|
| 60 | 21% | 25% |
| 65 | 19% | 23% |
| 70 | 17% | 21% |
Grade 60 is the most ductile of the three and Grade 70 the least. The two gauge lengths describe the same steel, and the shorter gauge concentrates the stretching, so its percentage is always higher. Your mill certificate will report whichever gauge the mill used.
Ductility matters most during fabrication rather than in service. If your vessel involves tight-radius forming, dished heads pressed from flat plate, or heavy cold work, the extra ductility of Grade 60 is genuinely useful. It matters again in service as a safety characteristic, because a ductile vessel yields and bulges where a harder one might crack.
Difference in Chemistry
The strength difference is created almost entirely by carbon content. Here are the maximum carbon limits by grade and thickness, based on heat analysis.
| Plate thickness | Grade 60 | Grade 65 | Grade 70 |
|---|---|---|---|
| Up to 12.5 mm | 0.21% | 0.24% | 0.27% |
| Over 12.5 to 50 mm | 0.23% | 0.26% | 0.28% |
| Over 50 to 100 mm | 0.25% | 0.28% | 0.30% |
| Over 100 mm | 0.27% | 0.29% | 0.31% |
Manganese also differs at the thin end. Grade 60 plate up to 12.5 mm allows 0.60 to 0.90% manganese, while Grades 65 and 70 require 0.85 to 1.20% across the board. Silicon, phosphorus and sulphur limits are identical for all three grades.
Two consequences follow from this table. First, the grades converge as plate gets thicker. At 25 mm the carbon gap between Grade 60 and Grade 70 is 0.05 percentage points, while at 120 mm it narrows to 0.04. Second, and more usefully, a thick Grade 60 plate carries more carbon than a thin Grade 70 plate. Grade is not a reliable shortcut for weldability on its own, and you have to read the certificate.
Difference in Toughness
This is the comparison most people get wrong, because the specification does not answer it directly.
Charpy V-notch impact testing is not a standard requirement for any A516 grade. It is a supplementary requirement, and if you do not write it on the purchase order, the mill will not test for it and your certificate will not report it. This is true for Grade 60 and Grade 70 alike.
That said, the metallurgy is clear. Lower carbon gives better notch toughness, so Grade 60 has a real inherent advantage over Grade 70 when both are supplied in the same condition. For cold-service vessels this is a legitimate reason to step down a grade.
Heat treatment matters more than grade, though. Normalizing refines the grain structure and improves low-temperature toughness far more than a grade change does. A normalized Grade 70 plate will comfortably outperform an as-rolled Grade 60 plate at low temperature. Plates over 40 mm are normalized as standard across all grades, but below that thickness you must specify normalizing yourself.
The order of priority is worth remembering. Specify the impact test first, then the heat treatment, and only then consider dropping a grade.
Difference Between SA 516 Gr 60 and 70
Grade 65 sits quietly in the middle, so in practice the real decision is almost always between the outer two. Here is that comparison in isolation.
| Point of comparison | SA 516 Gr 60 | SA 516 Gr 70 |
|---|---|---|
| Tensile strength | 415–550 MPa | 485–620 MPa |
| Yield strength, minimum | 220 MPa | 260 MPa |
| Elongation in 200 mm | 21% minimum | 17% minimum |
| Carbon, 25 mm plate | 0.23% max | 0.28% max |
| Allowable stress, ASME VIII-1 | 17.1 ksi | 20.0 ksi |
| Wall thickness for the same duty | Around 17% thicker | Thinner and lighter |
| Weldability | Easier, lower preheat demand | Good, preheat matters above 40 mm |
| Inherent notch toughness | Slightly better | Slightly lower |
| Market availability | Available on request | Stocked everywhere |
| Typical cost per tonne | Similar or marginally lower | Similar, often cheaper in practice |
A note on the prefix, since both forms appear on drawings and purchase orders. SA 516 is the ASME version of the grade and A516 is the ASTM version. The steel and the property requirements are the same, but if your vessel is being built to the ASME Boiler and Pressure Vessel Code, the purchase order and the mill certificate must both say SA-516. An A516 certificate alone will not satisfy a code inspector, so it is worth checking before the plate is cut, and the difference between the ASTM and ASME designations is worth understanding before you order.
The short version of the difference between SA 516 Gr 60 and 70 is that Grade 70 buys you a thinner, lighter vessel while Grade 60 buys you easier fabrication and a small toughness margin. For most projects the availability of Grade 70 settles it, which is why it dominates the market.
How Grade Choice Affects Wall Thickness and Cost
This is where the strength numbers become money.
Under ASME Section VIII Division 1, required wall thickness is inversely proportional to allowable stress. Grade 70 is rated at 20.0 ksi and Grade 60 at 17.1 ksi, a difference of about 17%. So for the same diameter, pressure and joint efficiency, a Grade 60 vessel needs roughly 17% more wall thickness than a Grade 70 vessel.
On a small vessel that might mean stepping from 12 mm to 14 mm, which nobody notices. On a large storage tank or a thick-walled reactor it means a significant increase in tonnage, more welding consumables, more welding hours, higher lifting and transport costs, and sometimes a change in whether post-weld heat treatment is required at all.
Price per tonne for the three grades is broadly similar, so the cheaper vessel is usually the one that uses less steel. That is the main commercial argument for Grade 70, and it holds for most vessels above modest size.
Weldability and Fabrication
All three grades weld well, which is one of the reasons A516 became the default pressure vessel plate. The differences are real but manageable.
Carbon equivalent is the number to watch. Grade 60 typically runs around 0.38 to 0.42, while Grade 70 runs around 0.43 to 0.45. A higher carbon equivalent means a greater risk of hydrogen-induced cold cracking in the heat-affected zone, which is controlled by preheat and by keeping hydrogen out of the weld.
Practical guidance is similar across the grades. Use low-hydrogen consumables, keep the plate surface dry and free of scale, and apply preheat as thickness increases. Preheat becomes important above roughly 40 mm for Grade 70, and the threshold sits somewhat higher for Grade 60.
Forming behaves as the elongation figures suggest. Grade 60 tolerates tighter bend radii and heavier cold work before cracking, so fabricators working on complex shapes sometimes prefer it even when the strength is not needed.
Applications: Where Each Grade Is Used
Grade 60 appears where toughness and formability matter more than strength. Typical uses include low-pressure storage vessels, cold-service equipment, vessels with heavily formed sections, and applications where the design is governed by something other than pressure, such as corrosion allowance or handling loads.
Grade 65 is the middle option and by far the least common. It gets specified when a design calculation lands awkwardly between the other two, or when an existing drawing or a client standard calls for it. Because stock is limited, lead times are often longer than for either neighbour.
Grade 70 is the industry default. It is used for pressure vessels and reactors in refineries and petrochemical plants, boiler drums, heat exchanger shells and tubesheets, LPG and ammonia storage, and large process tanks. If you are looking at ASTM A516 Grade 70 Plate for a vessel project, you are choosing the grade that mills stock in the widest thickness range and the one fabricators are most familiar with.
Which Grade Should You Specify?
Work through it in this order.
- Run the design calculation first. If Grade 60 satisfies the required thickness at an acceptable weight, it is a valid choice. If it forces an awkward plate thickness, step up.
- Check your service temperature. Below about 0 °C, specify impact testing and normalizing before you consider changing grade. Heat treatment does more for toughness than grade does.
- Consider the forming. Heavy cold work or tight radii favour Grade 60.
- Check availability and lead time. Grade 70 is stocked in more thicknesses and sizes than the other two combined, and Grade 65 is the hardest to source quickly.
- Compare total cost, not plate price. Less steel usually beats a marginally cheaper grade once welding and handling are counted.
For a straightforward pressure vessel with no unusual forming and no deep cold service, Grade 70 is the sensible default.
Common Mistakes When Comparing the Grades
- Assuming a lower grade automatically means better toughness. It helps, but normalizing and a specified Charpy test matter far more.
- Assuming impact testing is included in any grade. It is supplementary in all of them.
- Treating tensile strength as a minimum only. Every grade has an upper limit, and exceeding it is a rejection criterion.
- Choosing Grade 65 without checking stock. The saving rarely justifies the lead time.
- Writing A516 when the vessel is ASME-coded. The certificate needs to say SA-516.
- Comparing carbon by grade alone. A thick Grade 60 plate can carry more carbon than a thin Grade 70 plate.
Frequently Asked Questions
What is the main difference between A516 Grade 60 and Grade 70?
Grade 70 is stronger, with 485–620 MPa tensile strength and 260 MPa minimum yield against 415–550 MPa and 220 MPa for Grade 60. The trade-off is ductility, since Grade 70 requires only 17% elongation while Grade 60 requires 21%. In design terms, Grade 70 lets you build the same vessel with roughly 17% less wall thickness.
Is A516 Grade 70 better than Grade 60?
Not better, just different. Grade 70 is the right choice when weight, thickness or availability drive the decision, which covers most pressure vessel work. Grade 60 is better when the vessel involves heavy forming, or when its lower carbon content genuinely helps with weldability or cold-service toughness.
Why is Grade 65 so rarely used?
Its properties sit between two grades that are both easy to source, so it offers no clear advantage. Designers who need more than Grade 60 usually go straight to Grade 70 because stock is better and the price difference is small. As a result Grade 65 is often a special order with a longer lead time.
Do all three grades have the same chemical composition?
No. Carbon content is the main variable and it rises with each grade, from 0.21% maximum for thin Grade 60 plate up to 0.31% maximum for thick Grade 70 plate. Manganese differs on thin plate as well. Silicon, phosphorus and sulphur limits are identical for all three.
Which A516 grade is best for low-temperature service?
Grade 60 has a small inherent advantage because of its lower carbon, but the more effective levers are normalizing and specifying Charpy impact testing at your service temperature. A normalized Grade 70 plate with certified impact values will outperform an untested as-rolled Grade 60 plate. Decide the heat treatment and testing first, then the grade.
Can I substitute Grade 70 where Grade 60 is specified?
Usually yes on strength, since Grade 70 meets or exceeds every Grade 60 mechanical requirement. But check two things before you do. Confirm that the higher carbon content will not affect your welding procedure, and confirm that your design code or client specification permits the substitution in writing.
What is the allowable stress difference between the grades?
Under ASME Section VIII Division 1, allowable stress at ambient temperature is 17.1 ksi for Grade 60, 18.6 ksi for Grade 65 and 20.0 ksi for Grade 70. Each figure is the minimum tensile strength divided by a design margin of 3.5. All three fall as operating temperature rises.
Are SA 516 and A516 the same grade?
They describe the same steel with the same property requirements. A516 is the ASTM specification and SA-516 is its adoption into the ASME Boiler and Pressure Vessel Code. For code-stamped vessels the purchase order and the mill certificate must both name SA-516 explicitly.
Summary
The three A516 grades share one specification and differ mainly in strength. Grade 60 gives 415–550 MPa tensile and 21% elongation, Grade 65 gives 450–585 MPa and 19%, and Grade 70 gives 485–620 MPa and 17%. Every step up adds strength and removes ductility, driven by a small increase in carbon.
Grade 70 dominates because thinner walls mean less steel, and because mills stock it in more sizes than the other two combined. Grade 60 earns its place on vessels with heavy forming or where lower carbon simplifies welding. Grade 65 is a niche option worth checking stock on before you specify it.
Whichever grade you choose, remember that toughness is not part of the base specification. Impact testing and normalizing have to be written onto the purchase order, and they will do more for a cold-service vessel than any grade change.
Tell us your design temperature, thickness and service conditions and we will confirm the right grade, sizes and certification.